1. Introduction to die-casting

Pressure casting, referred to as die casting, is a casting method in which molten gold is poured into the pressure chamber to fill the cavity of a steel mold at high speed, and the molten alloy is solidified under pressure to form a casting.

The main feature that distinguishes die casting from other casting methods is high pressure and high speed. (1) The molten metal fills the cavity under pressure, and crystallizes and solidifies at a higher pressure, and the common pressure is 15-100MPa. (2) The molten metal fills the cavity at high speed, usually at 10-50 m/s, and some can exceed 80 m/s, (the linear velocity of the cavity introduced through the inner gate - the velocity of the inner gate), so the filling time of the molten metal is very short, about 0.01-0.2 seconds (depending on the size of the casting) can fill the cavity.

Die-casting machine, die-casting alloy and die-casting mold are the three major elements of die-casting production, all of which are indispensable. The so-called die-casting process is to organically and comprehensively use these three elements to enable the stable rhythmic and efficient production of qualified castings with good appearance, intrinsic quality, and dimensions that meet the requirements of drawings or agreements, and even high-quality castings.

1. Die-casting machine

(1) Classification of die-casting machines

The heating conditions of the press chamber of the die-casting machine can be divided into two categories: hot pressing chamber and cold pressing chamber. The pressure chamber and the mold placement position are different, and the cold chamber die-casting machine can be divided into three forms of die-casting machine: vertical, horizontal and fully vertical.


(2) The main parameters of the die-casting machine


2. Die-casting alloy

The alloys used in die castings are mainly non-ferrous alloys, and ferrous metals (steel, iron, etc.) are rarely used at present due to problems such as mold materials. Among the non-ferrous alloy die castings, aluminum alloy is widely used, followed by zinc alloy.

The following is a brief introduction to the situation of die-casting non-ferrous metals.

(1) Classification of die-casting non-ferrous alloys


2. Die-casting mold

Die-casting mold is one of the three major elements of die-casting production, and the correct and reasonable structure of the mold is a prerequisite for the smooth progress of die-casting production, and plays an important role in ensuring the quality of castings (off-machine pass rate).

Due to the characteristics of the die-casting process, the correct selection of each process parameter is the decisive factor to obtain high-quality castings, and the mold is the premise of being able to correctly select and adjust the process parameters, and the mold design is essentially a comprehensive reflection of the various factors that may occur in the die-casting production. If the mold design is reasonable, there are few problems encountered in the actual production, and the pass rate of castings is high. On the contrary, the mold design is unreasonable, for example, the wrapping force of the dynamic fixed mold is basically the same when the casting is designed, and the gating system is mostly produced on the Guannan die-casting machine that the fixed mold cannot be fed by the punch after injection, and the casting cannot be produced normally, and the casting has been glued to the fixed mold. Although the finish of the fixed cavity is very smooth, due to the deep cavity, there is still a phenomenon of sticking to the fixed mold. Therefore, in the mold design, it is necessary to comprehensively analyze the structure of the casting, be familiar with the operation process of the die-casting machine, understand the possibility of adjusting the die-casting machine and process parameters, master the filling characteristics in different situations, and consider the mold processing method, drilling hole and fixed form, in order to design a realistic mold that meets the production requirements.

As mentioned at the beginning, the filling time of molten metal is extremely short, the specific pressure and flow rate of molten metal are very high, which is extremely harsh for the working conditions of the die-casting mold, coupled with the impact of alternating stress of quenching and heat, which has a great impact on the service life of the mold.

The service life of a mold usually refers to the number of die-cast modules (including the number of scrap products in die-casting production) that occurs through careful design and manufacturing, under normal use conditions, combined with good maintenance, and before it can no longer be repaired and scrapped.

In actual production, there are three main forms of mold failure: (1) thermal fatigue crack damage failure; (2) fragmentation failure; (3) Dissolution failure.

There are many factors that cause the mold to fail, including external factors (such as the casting temperature, whether the mold has been preheated, the amount of water agent paint sprayed, whether the tonnage of the die-casting machine is matched, the die-casting pressure is too high, the inner gate speed is too fast, the cooling water is not synchronized with the die-casting production, the type and composition of the casting material and the level of Fe, the size and shape of the casting, the wall thickness, the type of coating, etc.). There are also internal factors (such as the metallurgical quality of the material of the mold itself, the forging process of the blank, the rationality of the mold structure design, the rationality of the gating system design, the internal stress generated during the processing of the mold machine (electrical processing), the heat treatment process of the mold, including various fitting accuracy and finish requirements, etc.).

If there is an early failure of the mold, it is necessary to find out what internal or external causes are so that it can be improved in the future.

(1) Thermal fatigue cracking failure of the mold

During the production of die-casting, the mold is repeatedly subjected to the action of cold and heat, and the forming surface and its interior are deformed, and the thermal stress of repeated cycles occurs due to mutual involvement, resulting in the second damage and loss of toughness of the tissue structure, causing the appearance of microcracks, and continuing to expand.

For this reason, on the one hand, the mold must be fully preheated at the beginning of die casting. In addition, the mold must be kept within a certain operating temperature range during the die casting production process to avoid early cracking failure. At the same time, it is necessary to ensure that there are no problems with internal factors before the mold is put into production and during manufacturing. In actual production, most of the mold failures are thermal fatigue crack failures.

(2) Fragmentation failure

Under the action of ejection force, cracks will erupt in the weakest part of the mold, especially the marking marks or electromachining marks on the forming surface of the mold have not been polished, or the clear corners of the molding will be the first to appear fine cracks, and when there is a brittle phase or coarse grains in the grain boundary, it is easy to fracture. The crack propagation is rapid during brittle fracture, which is a dangerous factor for the fragmentation and failure of the mold. For this reason, on the one hand, all scratches and electrical processing marks on the mold surface must be polished, even if it is in the gating system part. In addition, the mold materials used are required to have high strength, good plasticity, good impact toughness and fracture toughness.

(3) Melt failure

As mentioned earlier, the commonly used die-casting alloys are zinc alloy, aluminum alloy, magnesium alloy and copper alloy, as well as pure aluminum die-casting, Zn, Al, Mg are more active metal elements, they have a good affinity with the mold material, especially Al easy to bite the mold. When the hardness of the mold is high, the corrosion resistance is better, and if there are soft spots on the forming surface, the corrosion resistance is not good. However, in actual production, dissolution is only a local part of the mold, and the parts (core, cavity) directly washed by the gate are prone to dissolution, and the soft hardness is prone to the appearance of aluminum alloy sticking mold.

Points to note about the problems that often exist in die casting production:

1. Gating system and overflow system

example

(1) Requirements for mold sprue on cold chamber horizontal die-casting machine:

(1) The diameter of the pressure chamber should be selected according to the required specific pressure and the fullness of the pressure chamber, and at the same time, the inner diameter deviation of the gate sleeve should be appropriately enlarged by a few wires compared with the deviation of the diameter of the pressure chamber, so as to avoid the problem of punch jamming or serious wear caused by the different shafts of the gate sleeve and the diameter of the pressure chamber, and the wall thickness of the gate sleeve should not be too thin. The length of the sprue sleeve should generally be smaller than the ejection lead of the injection punch so that the paint can be removed from the chamber.

(2) The inner hole of the pressure chamber and the gate sleeve should be finely ground after heat treatment, and then ground along the axis, and its surface roughness should be ≤ Ra0.2μm

(3) The recess depth of the diverter and the cavity that forms the paint is equal to the depth of the cross sprue, and its diameter is matched with the inner diameter of the gate sleeve, and there is a 5° slope along the demoulding direction. When a coated sprue is used, the volume of the effective length of the chamber is shortened, and the filling degree of the chamber can be improved.

(2) Requirements for mold cross sprue

(1) The entrance of the horizontal sprue of the cold horizontal mold should generally be located at the upper inner diameter of the pressure chamber more than 2/3 of the part, so as to prevent the molten metal in the press chamber from entering the sprue prematurely under the action of gravity and starting to solidify in advance.

(2) The cross-sectional area of the sprue should be gradually reduced from the sprue to the inner gate, and in order to expand the cross-section, negative pressure will occur when the molten metal flows through, which is easy to inhale the gas on the parting surface and increase the eddy current encapsulation in the flow of molten metal. Generally, the cross-section of the outlet is 10-30% smaller than that of the inlet.

(3) The sprue should have a certain length and depth. The purpose of maintaining a certain length is to play the role of stabilizing the flow and guiding. If the depth is not enough, the molten metal will cool down quickly, and if the depth is too deep, the condensation will be too slow, which will not only affect the productivity but also increase the amount of return material.

(4) The cross-sectional area of the cross-sprue should be greater than the cross-sectional area of the inner gate to ensure the speed of metal liquid entering the mold. The cross-sectional area of the main cross-sprue should be greater than the cross-sectional area of each branch cross-sprue.

(5) The bottom two sides of the sprue should be rounded to avoid early cracks, and the two sides can be made with an inclination of about 5°. The surface roughness of the crossrunner part ≤ Ra0.4μm

(3) Inner gates

(1) The parting surface should not be closed immediately after the molten metal enters the mold, and the overflow groove and exhaust groove should not hit the core head-on. The flow direction of the liquid metal into the mold is as much as possible along the rib bar and heat sink that are cast, and the thick wall is filled from the thin wall.

(2) When selecting the location of the inner gate, the flow of molten metal should be as shortest as possible. When using multi-strand inner gate, it is necessary to prevent several strands of molten metal from converging and impacting each other after entering the mold, resulting in defects such as eddy current gas encapsulation and oxidation inclusion.

(3) The thickness of the inner gate of the thin-walled part should be appropriately small to ensure the necessary filling speed, and the setting of the inner gate should be convenient for removal, and the casting body should not be defective (eat meat).

(4) Overflow groove

(1) The overflow groove should be easy to remove from the casting, and try not to damage the casting body.

(2) When setting an exhaust groove on the overflow groove, it is necessary to pay attention to the position of the overflow port to avoid blocking the exhaust groove prematurely and making the exhaust groove ineffective.

(3) Several overflow ports or a very wide and thick overflow port should not be opened on the same overflow groove, so as to avoid the cold liquid, slag, gas, and paint in the molten metal from returning to the cavity from the overflow groove, resulting in casting defects.

2. Casting fillet (including corners)

The casting diagram often indicates that the fillet R2 and other requirements are not indicated, and we must not ignore the role of these unmarked fillet when opening the mold, and never make a clear corner or too small fillet angle. The casting fillet can make the molten metal filling smooth, so that the gas in the cavity can be discharged sequentially, and can reduce the stress concentration and prolong the service life of the mold. (Castings are also not prone to cracks or various defects due to poor filling). For example, there are more clear corners on the standard oil pan die, relatively speaking, the brother oil pan die is the best at present, and there are more heavy engine oil pans.

3. Demoulding slope

It is strictly forbidden to have artificially caused side concave in the demoulding direction (often the casting is stuck in the mold during the mold test, and when it is treated in an incorrect way, such as drilling, hard chisel, etc., the local concave is made)

4. Surface roughness

The molding part and the gating system should be carefully polished as required, and should be polished along the demoulding direction. Since the molten metal enters the gating system from the pressure chamber and fills the cavity, the entire process takes only 0.01-0.2 seconds. In order to reduce the resistance of the molten metal flow and minimize the pressure loss, it is necessary to have a high finish on the surface through which it flows. At the same time, the heating and erosion conditions of the gating system are harsh, and the worse the finish, the more easily the mold is damaged.

5. The hardness of the mold forming part

Aluminum alloy: HRC46°

Copper: HRC around 38°

When processing, the mold should try to leave a margin for repair, make the upper limit of the size, and avoid welding.

Technical requirements for die casting mold assembly:

1. The requirement of the parallelism between the parting surface of the mold and the plane of the template.

2. Requirements for the perpendicularity of the guide pillar, guide sleeve and template.

3. The plane of the moving and fixed mold insert on the parting surface and the moving fixed mold sleeve plate are 0.1-0.05mm higher

4. The push plate and reset rod are flush with the parting surface, and the general push rod is concave 0.1mm or according to user requirements.

5. All the moving parts on the mold are reliably moving, and there is no sluggishness and no string movement.

6. The positioning of the slider is reliable, the distance between the slider and the casting is kept when the core is withdrawn, and the matching part of the slider and the block is more than 2/3 after clamping.

7. The roughness of the sprue is smooth and seamless.

8. The local gap of the parting surface of the insert is < 0.05mm when clamping.

9. The cooling water channel is unblocked, and the import and export signs are marked.

10. The roughness of the forming surface is Rs=0.04, and there is no slight injury.